> My Expedition had a perfect finish, the glass came out crystal clear, the
> epoxy cured perfectly.... but about a month later after I had already
> taken the kayak out I noticed a small area where the cloth apeared to have
> raised, showing the texture of the weave. It was a perfect boat but now it
> has a small blemish on the deck. Is this what they call telegraphing? And
> does anyone know how to prevent this from happening on my next kayak.
> Also, I have a strip built canoe that I built recently. I noticed when I
> took it out of the water the other day that it had a silver dollar sized
> area that had delaminated in the hull area.I didnt appear to be their when
> I put it in the water. I store all my boats indoors while not in use, but
> the building does get into the 100's in the summer. I put 5 coats of spar
> varnish with uv and the only time the hull is exposed to the sun is when
> it's upside down on the back of my truck. I don't think I hit a rock or
> bumped the area in any way. Could it be that I didnt clean the area well
> enough before laying on the first coat of epoxy? I've dripped epoxy on the
> cement floor on top of saw dust, dirt etc.. and it bonds so well I can't
> get it of with a floor scraper. I know over exposure to uv can cause
> delamination but I don,t think that is the case here...
> Does anyone know what may have caused this so I can keep it from happening
> again?
> Regard Jim Burnell
My guess is that, somehow the wood or glass got contaminated and ruined the bond. Another possibility might be a high moisture content in the wood while glassing and then the wood outgassed the moisture in the hot sun. I have also been told, by Jo Greenley, that some epoxies don't hold up as well in the heat as well as others do. He said that MAS does better in the heat than System Three. What kind of epoxy are you using.
Mike
Messages In This Thread
- Telegraphing and delamination
Jim Burnell -- 8/23/1999, 9:37 pm- Delamination
Robert Woodard -- 8/24/1999, 9:19 pm- Re: Telegraphing and delamination
Mike Hanks -- 8/24/1999, 12:27 pm- Re: Telegraphing and delamination
Dave Houser -- 8/24/1999, 3:00 am - Re: Telegraphing and delamination
- Delamination